永磁感应辊式强磁机选别钴土矿工业试验

来源 :有色金属(冶炼部分) | 被引量 : 0次 | 上传用户:hsq650
下载到本地 , 更方便阅读
声明 : 本文档内容版权归属内容提供方 , 如果您对本文有版权争议 , 可与客服联系进行内容授权或下架
论文部分内容阅读
易门铜矿老厂钴矿原设计为单一浮选流程,其设计指标为:原矿品位0.133%,精矿品位1.2%,回收率65%。由于原矿中含有-0.074毫米占60%以上的大量原生矿泥,因此给浮选生产带来严重困难,不仅药剂消耗量大,工艺条件要求严,而且矿浆需要加温至30~40℃。生产实践表明,其试生产的最好指标仅达到回收率35%、精矿品位 The original copper plant of Yimen Copper Mine was originally designed as a single flotation process. Its design indexes are: raw ore grade of 0.133%, concentrate grade of 1.2% and recovery rate of 65%. As the raw ore contains a large amount of native slime with a mass fraction of -0.074 mm accounting for more than 60%, the flotation process poses serious difficulties for the flotation production. Not only the consumption of reagents is high, but the process conditions are strict, and the slurry needs to be warmed to 30-40 ° C. Production practice shows that the best indicators of its pilot production only reached 35% recovery rate, concentrate grade
其他文献
由于能源的减少和能价的升高,各工业都在认真考虑能源问题,铜工业也不例外。现有铜金属的主要工业生产方法有四种,即:反射炉熔炼,电炉熔炼,诺兰达法和奥托昆布闪速熔炼,现从
能否用铝矿石直接制取合格的氯化铝,是新法炼铝的关键问题之一,也是化工部门提出的一个课题。我们从1976年开始,对铝矿石沸腾氯化的工艺条件进行了小型试验研究,试验内容包
从散状物料中取样,其颗粒形状、密度、成分,假比重和有色泽都会变化,在含水(旦力)的比例上或颗粒表(?)吸收的其他液体含(旦力)也会不同。这些和其他的一些变(旦力)决定固体
近年来,为了满足各工业交通部门对钢材的质量和性能提出的越来越严格的要求,国内外采用了许多炉外精炼方法。钢包内吹氩气处理钢水(简称吹氩)是其中的一种。这种方法装置简
无氰选矿是选矿工业的重大革新,是有色选矿的发展方向,对环境保护有重大意义。矿党委对选矿中使用氰化物污染环境的问题非常重视,在批林批孔运动的推动下,根据上级指示精神,
过去三、四年以来,能源价格猛涨,1975年产生世界范围内的经济萎缩,基本金属的价格下跌,生产过程中,能源消耗大的金属,包括铝、镁和镍,尽管需求疲软,价格却没有下跌,甚至还涨
假定有一位年轻人,从现在开始能够定期每年存下1.4万元,如此持续40年。如果他每年存下的钱都能投资到股票或房地产,并获得每年平均20%的技资报酬率,那么40年后,他能积累多少
吉林铁合金厂在冶炼钨铁时,自收尘系统中每年可回收粉尘(即钨尘)约100~150吨。这种钨尘粒度较细,—320目的占80%。其代表试样成分为(%):WO_350.10;P0.11;S0.62;SiO.2 11.0;Ca 6
请下载后查看,本文暂不支持在线获取查看简介。 Please download to view, this article does not support online access to view profile.
杭州化工机械一厂制造的PF型盘式过滤机、FY型浸没泵和透平搅拌桨,是由具有20多年设计经验的专业设计院——南京化学工业公司设计院设计的。该设计既总结了国内同类产品的优