论文部分内容阅读
高锰钢水(革刃)的方法,一般是把高锰钢铸件放在平车上,推入加热炉加热至1050℃~1100℃,保持1~2小时,然后用卷扬机或吊车将平车自加热炉拖出至水池旁边,用吊车将平车一侧吊起,使平车倾侧,铸件即落入水中。这种方法从开启加热炉门至铸件倾入水中约需2分钟,如果在室外进行水(革刃)而天气又较冷时,这项工作就此较困难,因为时间长,温度降低太快,如果水(革刃)温度低於1000℃,对质量就有很大影响。
High manganese steel water (leather edge) method is generally high manganese steel castings on the flat car, pushed into the heating furnace heated to 1050 ℃ ~ 1100 ℃, for 1 to 2 hours, and then winch or crane flat car from Hearth dragged to the pool next to the crane side of the hoist will be hoisted flat car tilting, casting that falls into the water. This method takes about 2 minutes from opening the oven door to pouring the castings into the water. This work is more difficult if water (leather edges) are used outdoors and when the weather is colder because of the long time, the temperature drops too fast, If the water (leather edge) temperature below 1000 ℃, have a great impact on the quality.