论文部分内容阅读
Longquan celadon was prepared using local purple gold raw as blue glaze stain.X-Ray fluorescence analysis,X-ray diffraction analysis,and scanning electron microscopy were conducted to study the chemical composition and porcelain microstructure of different purple gold raw samples.Results showed that the glaze color of purple gold raw with 8.02 wt.% iron No.1 is grayish green and the glazed surface is bright under the same preparation conditions.Given the iron contents of No.2 (4.77 wt.%) and No.3 (5.20 wt.%),the glaze of these samples is light grayish green and light pink cyan,respectively.